A bracket in DMLS 316L Stainless Steel, as-sintered finish.

Mechanical
Yield strength530MPa1
Ultimate tensile strength640MPa1
Elongation at break40%1
Young's modulus (stiffness)185GPa2
Densitypart density7,900kg/m³3
Strength to weight67.1kN·m/kg
Stiffness to weight23.4MN·m/kg
Poisson's ratiobase material0.34
Shear modulus71.2GPa
Bulk modulus154GPa
Speed of sound4,839m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS 316L Stainless Steel
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS 316L Stainless Steel
Strength against densityHigher and further left: stronger for its weight
Thermal
Thermal conductivitybase material16.2W/m·K5
Thermal expansionmean 25-100 °C15.7µm/m·K1
100 mm part over a 50 °C swing78.6µm growth
Specific heatbase material500J/kg·K5
Heats up and cools (diffusivity)4.1mm²/s
Thermal shock resistance2,067W/m
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS 316L Stainless Steel
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30DMLS 316L Stainless Steel
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Sources5 documents: EOS GmbH, Steel Construction Institute, Cleveland-Cliffs
Values for
3D printed metal (DMLS). EOS StainlessSteel 316L (powder 9011-0032), EOS M 290, ParameterSet 316L 20µm Surface M290/400W, as manufactured, horizontal; ISO 6892-1
  1. 1
    EOS StainlessSteel 316L Material Data SheetEOS GmbHarchived copyYield strength: typical, as manufactured, horizontalUltimate tensile strength: typical, as manufactured, horizontalElongation at break: typical at break, as manufactured, horizontalThermal expansion: mean 25-100 °C, ASTM E228
  2. 2
    EOS StainlessSteel 316L Material Data Sheet, M 280 and M 290 (2014)EOS GmbHarchived copyYoung's modulus (stiffness): typical, as built, horizontal (XY); EOSINT M280-400W / M290-400W, 316L_Surface 1.0, 20 µm (2014 sheet)
  3. 3
    EOS StainlessSteel 316L Material Data Sheet, FlexLine, M 290 (2016)EOS GmbHarchived copyDensity: part density (ISO 3369, not labelled min or typical), EOS M 290, 40 µm FlexLine
  4. 4
    Design Manual for Structural Stainless Steel, 4th Edition (P413)Steel Construction Institutearchived copyPoisson's ratio: base material: austenitic stainless steels incl. 1.4404 (316L), design value
  5. 5
    316/316L Stainless Steel Product Data Bulletin (2021)Cleveland-CliffsThermal conductivity: base material: wrought 316/316L (Cleveland-Cliffs), at 100 °CSpecific heat: base material: wrought 316/316L (Cleveland-Cliffs), 0-100 °C

DMLS 316L Stainless Steel is 3D printed: its properties depend on build direction and print settings; these are typical values.

Thermal properties of DMLS 316L Stainless Steel

Thermal conductivity of DMLS 316L Stainless Steel

DMLS 316L Stainless Steel has a thermal conductivity of 16.2 W/m·K (9.36 BTU/hr·ft·°F). Basis: base material: wrought 316/316L (Cleveland-Cliffs), at 100 °C. Source: Cleveland-Cliffs, 316/316L Stainless Steel Product Data Bulletin (2021).

Specific heat of DMLS 316L Stainless Steel

The specific heat capacity of DMLS 316L Stainless Steel is 500 J/kg·K (0.119 BTU/lb·°F). Basis: base material: wrought 316/316L (Cleveland-Cliffs), 0-100 °C. Source: Cleveland-Cliffs, 316/316L Stainless Steel Product Data Bulletin (2021).

Coefficient of thermal expansion of DMLS 316L Stainless Steel

DMLS 316L Stainless Steel expands 15.7 µm/m·K (8.73 µin/in·°F): a 100 mm part grows 78.6 µm over a 50 °C rise. Basis: mean 25-100 °C, ASTM E228. Source: EOS GmbH, EOS StainlessSteel 316L Material Data Sheetarchived copy.

Thermal diffusivity of DMLS 316L Stainless Steel

Computed from the conductivity, density and specific heat (k / ρc): 4.1 mm²/s, how fast a temperature change spreads through it.

Compare DMLS 316L Stainless Steel with