Materials / Compare

FDM ASA vs. Plastic Nylon PA66

Compare FDM ASA vs. Plastic Nylon PA66 strength, stiffness, weight and thermal properties.

FDM ASA3D printed (FDM)
Plastic Nylon PA66Bulk polymer (molded or machined)
MechanicalFDM ASAPlastic Nylon PA66
Yield strengthnot given (tensile used)85MPa1
Ultimate tensile strength37MPa2not stated (yield given)
Flexural strength65MPa2not sourced
Elongation at break9.2%230%13.26x more ductile
Young's modulus (stiffness)2.45GPa23GPa122% stiffer
Density1,050kg/m³21,130kg/m³1
Strength to weight35.2kN·m/kg75.2kN·m/kg2.13x higher
Stiffness to weight2.33MN·m/kg2.65MN·m/kg14% higher
Poisson's rationot sourcedbase material0.43
Shear modulusnot sourced1.07GPa
Bulk modulusnot sourced5GPa
Speed of sound1,528m/s1,629m/s7% faster
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM ASAPlastic Nylon PA66
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM ASAPlastic Nylon PA66
Strength against densityHigher and further left: stronger for its weight
ThermalFDM ASAPlastic Nylon PA66
Thermal conductivitybase material0.17W/m·K40.33W/m·K11.94x more heat through a fin
Thermal expansionbase material80–110µm/m·K4longitudinal98µm/m·K1
100 mm part over a 50 °C swing475µm growth3% less490µm growth
Specific heatnot sourced1,700J/kg·K1
Heats up and cools (diffusivity)not sourced0.172mm²/s
Thermal shock resistancenot sourced57.2W/m
Melting pointnot sourcedDSC260°C1
Max service temperatureHDT 1.8 MPa92°C2101°C1
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM ASAPlastic Nylon PA66
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM ASAPlastic Nylon PA66
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: BASF, Bambu Lab, Covestro, INEOS Styrolution
FDM ASA
Bambu Lab ASA, TDS V3.0, printed specimens X-Y; nozzle 260 °C, bed 80 °C, 200 mm/s, 100% infill; annealed and dried 80 °C for 12 h before testing.
Plastic Nylon PA66
BASF Ultramid A3K (PA66, unreinforced injection-moulding grade), Product Information 02/2026, dry values (ISO methods)
  1. 1
    Ultramid A3K Product InformationBASFPlastic Nylon PA66 · Yield strength: typical, dryPlastic Nylon PA66 · Elongation at break: nominal strain at break, dryPlastic Nylon PA66 · Young's modulus (stiffness): typical, dryPlastic Nylon PA66 · Density: typicalPlastic Nylon PA66 · Thermal conductivity: typicalPlastic Nylon PA66 · Thermal expansion: longitudinal, 23-55 °CPlastic Nylon PA66 · Specific heat: typicalPlastic Nylon PA66 · Melting point: DSCPlastic Nylon PA66 · Max service temperature: IEC 60216 temperature index, 20000 h
  2. 2
    Bambu ASA Technical Data Sheet, V3.0Bambu LabFDM ASA · Ultimate tensile strength: typicalFDM ASA · Flexural strength: typicalFDM ASA · Elongation at break: typicalFDM ASA · Young's modulus (stiffness): typicalFDM ASA · Density: typicalFDM ASA · Max service temperature: HDT 1.8 MPa
  3. 3
    Engineering Polymers Part and Mold Design: Thermoplastics, A Design GuideCovestroPlastic Nylon PA66 · Poisson's ratio: base material: unfilled polyamide (PA), conditioned, maker design-guide family value (Covestro Table 3-1)
  4. 4
    Luran S 777K (ASA) Product Data SheetINEOS StyrolutionFDM ASA · Thermal conductivity: base material: INEOS Styrolution Luran S 777K injection-molding ASA, typicalFDM ASA · Thermal expansion: base material: INEOS Styrolution Luran S 777K injection-molding ASA, range

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

FDM ASA is 3D printed: its properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is FDM ASA stronger than Plastic Nylon PA66?

Plastic Nylon PA66 is stronger: its yield strength is 85 MPa against tensile strength 37 MPa for FDM ASA (2.3x).

Which is lighter, FDM ASA or Plastic Nylon PA66?

FDM ASA is lighter: 1,050 kg/m³ against 1,130 kg/m³ for Plastic Nylon PA66.

Which is stiffer, FDM ASA or Plastic Nylon PA66?

Plastic Nylon PA66 is stiffer: Young's modulus 3 GPa against 2.45 GPa for FDM ASA, so the same part in Plastic Nylon PA66 deflects less under the same load.

Which is lighter for the same job, FDM ASA or Plastic Nylon PA66?

For the same stiffness or strength: Plastic Nylon PA66 is lighter for a stiff rod or tie (tension), stiff beam (bending), strong rod or tie, strong beam, strong panel or plate.

Part that must beFDM ASAPlastic Nylon PA66
Stiff rod or tie (tension)14% heavierlighter
Stiff beam (bending)3% heavierlighter
Stiff panel or plateabout equalabout equal
Strong rod or tie2.13x heavierlighter
Strong beam1.62x heavierlighter
Strong panel or plate41% heavierlighter

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, FDM ASA or Plastic Nylon PA66?

Plastic Nylon PA66 stretches further before it breaks: 30% elongation at break against 9.2% for FDM ASA.

Thermal

Which conducts heat better, FDM ASA or Plastic Nylon PA66?

Plastic Nylon PA66 conducts heat better: 0.33 W/m·K against 0.17 W/m·K for FDM ASA.

Which expands less with temperature?

FDM ASA expands less: 95 µm/m·K against 98 µm/m·K for Plastic Nylon PA66.

Related comparisons