Materials / Compare

FDM ASA vs. Plastic PETG

Compare FDM ASA vs. Plastic PETG strength, stiffness, weight and thermal properties.

FDM ASA3D printed (FDM)
Plastic PETG3D printed (FDM)
MechanicalFDM ASAPlastic PETG
Yield strengthnot given (tensile used)46.2MPa1
Ultimate tensile strength37MPa246.2MPa125% stronger
Flexural strength65MPa278.9MPa121% stronger in bending
Elongation at break9.2%221% more ductile7.6%1
Young's modulus (stiffness)2.45GPa226% stiffer1.94GPa1
Density1,050kg/m³221% lighter1,270kg/m³1
Strength to weight35.2kN·m/kg36.4kN·m/kg3% higher
Stiffness to weight2.33MN·m/kg1.53x higher1.53MN·m/kg
Poisson's rationot sourcednot sourced
Shear modulusnot sourcednot sourced
Bulk modulusnot sourcednot sourced
Speed of sound1,528m/s24% faster1,236m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM ASAPlastic PETG
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM ASAPlastic PETG
Strength against densityHigher and further left: stronger for its weight
ThermalFDM ASAPlastic PETG
Thermal conductivitybase material0.17W/m·K3base material0.21W/m·K424% more heat through a fin
Thermal expansionbase material80–110µm/m·K3base material51µm/m·K4
100 mm part over a 50 °C swing475µm growth255µm growth1.86x less
Specific heatnot sourcedbase material1,300J/kg·K4
Heats up and cools (diffusivity)not sourced0.127mm²/s
Thermal shock resistancenot sourcednot sourced
Glass transitionnot sourced77.4°C1
Max service temperatureHDT 1.8 MPa92°C2HDT 0.455 MPa76.2°C1
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM ASAPlastic PETG
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30FDM ASAPlastic PETG
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: UltiMaker, Bambu Lab, INEOS Styrolution, Eastman
FDM ASA
Bambu Lab ASA, TDS V3.0, printed specimens X-Y; nozzle 260 °C, bed 80 °C, 200 mm/s, 100% infill; annealed and dried 80 °C for 12 h before testing.
Plastic PETG
Ultimaker PETG, 3D-printed specimens, XY (flat); Ultimaker S5 Pro, engineering intent profile, 0.15 mm layer height, AA 0.4 print core, 100% infill, Cura 4.9, printed one-at-a-time, conditioned >=24 h at room temperature. TDS v1.00, April 29, 2022.
  1. 1
    Ultimaker PETG Technical Data Sheet, v1.00UltiMakerarchived copyPlastic PETG · Yield strength: typicalPlastic PETG · Ultimate tensile strength: typical, peak stress (= stress at yield)Plastic PETG · Flexural strength: typicalPlastic PETG · Elongation at break: typicalPlastic PETG · Young's modulus (stiffness): typicalPlastic PETG · Density: typicalPlastic PETG · Glass transition: typicalPlastic PETG · Max service temperature: HDT 0.455 MPa (printed specimens)
  2. 2
    Bambu ASA Technical Data Sheet, V3.0Bambu LabFDM ASA · Ultimate tensile strength: typicalFDM ASA · Flexural strength: typicalFDM ASA · Elongation at break: typicalFDM ASA · Young's modulus (stiffness): typicalFDM ASA · Density: typicalFDM ASA · Max service temperature: HDT 1.8 MPa
  3. 3
    Luran S 777K (ASA) Product Data SheetINEOS StyrolutionFDM ASA · Thermal conductivity: base material: INEOS Styrolution Luran S 777K injection-molding ASA, typicalFDM ASA · Thermal expansion: base material: INEOS Styrolution Luran S 777K injection-molding ASA, range
  4. 4
    Eastar Copolyester 6763 Product Data SheetEastmanPlastic PETG · Thermal conductivity: base material: Eastman Eastar Copolyester 6763 (PETG), typicalPlastic PETG · Thermal expansion: base material: Eastman Eastar Copolyester 6763 (PETG), typicalPlastic PETG · Specific heat: base material: Eastman Eastar Copolyester 6763 (PETG), DSC at 60 °C (lowest temperature listed)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

FDM ASA and Plastic PETG are 3D printed: their properties depend on build direction and print settings; these are typical values.

Questions

Mechanical

Is FDM ASA stronger than Plastic PETG?

Plastic PETG is stronger: its yield strength is 46.2 MPa against tensile strength 37 MPa for FDM ASA (25%).

Which is lighter, FDM ASA or Plastic PETG?

FDM ASA is lighter: 1,050 kg/m³ against 1,270 kg/m³ for Plastic PETG.

Which is stiffer, FDM ASA or Plastic PETG?

FDM ASA is stiffer: Young's modulus 2.45 GPa against 1.94 GPa for Plastic PETG, so the same part in FDM ASA deflects less under the same load.

Which is lighter for the same job, FDM ASA or Plastic PETG?

For the same stiffness or strength: FDM ASA is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong beam, strong panel or plate; Plastic PETG is lighter for a strong rod or tie.

Part that must beFDM ASAPlastic PETG
Stiff rod or tie (tension)lighter1.53x heavier
Stiff beam (bending)lighter36% heavier
Stiff panel or platelighter31% heavier
Strong rod or tie3% heavierlighter
Strong beamlighter4% heavier
Strong panel or platelighter8% heavier

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, FDM ASA or Plastic PETG?

FDM ASA stretches further before it breaks: 9.2% elongation at break against 7.6% for Plastic PETG.

Thermal

Which conducts heat better, FDM ASA or Plastic PETG?

Plastic PETG conducts heat better: 0.21 W/m·K against 0.17 W/m·K for FDM ASA.

Which expands less with temperature?

Plastic PETG expands less: 51 µm/m·K against 95 µm/m·K for FDM ASA.

Related comparisons