Materials / Titanium

Titanium Ti-6Al-4V

Titanium Ti-6Al-4V (Grade 5, annealed) strength, stiffness, density and thermal properties, with their source.

A bracket in Titanium Ti-6Al-4V, brushed finish.

Mechanical
Yield strength885MPa1
Ultimate tensile strength940MPa1
Elongation at break16%1
Young's modulus (stiffness)107–122GPa2
Density4,430kg/m³1
Strength to weight200kN·m/kg
Stiffness to weight25.8MN·m/kg
Poisson's ratio0.3421
Shear modulus42.7GPa
Bulk modulus121GPa
Speed of sound5,084m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Brass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Titanium Ti-6Al-4V
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Brass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Titanium Ti-6Al-4V
Strength against densityHigher and further left: stronger for its weight
Thermal
Thermal conductivity6.6W/m·K2
Thermal expansion9µm/m·K2
100 mm part over a 50 °C swing45µm growth
Specific heat580J/kg·K2
Heats up and cools (diffusivity)2.57mm²/s
Thermal shock resistance3,730W/m
Melting pointmelting range1,630–1,650°C1
Max service temperature400°C1
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Brass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Titanium Ti-6Al-4V
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Brass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Titanium Ti-6Al-4V
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Sources2 documents: TIMET
Values for
Wrought. TIMETAL 6-4 (Ti-6Al-4V Grade 5) annealed plate typical (TIMET properties manual) + TIMET datasheet TMC-0150 physical properties
  1. 1
    TIMETAL 6-4 PropertiesTIMETarchived copyYield strength: typical, plate (>0.187 in), annealed, 0.2% offsetUltimate tensile strength: typical, plate, annealedElongation at break: typical, in 2 in., plate annealedDensity: nominalPoisson's ratio: mean of TIMET measurementsMelting point: melting rangeMax service temperature: upper recommended use temperature
  2. 2
    TIMETAL 6-4 Data SheetTIMETarchived copyYoung's modulus (stiffness): typical range, 20 °CThermal conductivity: typical, 20 °C, mill annealedThermal expansion: typical, mean 0-100 °CSpecific heat: typical, 20 °C

Thermal properties of Titanium Ti-6Al-4V

Thermal conductivity of Titanium Ti-6Al-4V

Titanium Ti-6Al-4V has a thermal conductivity of 6.6 W/m·K (3.81 BTU/hr·ft·°F). Basis: typical, 20 °C, mill annealed. Source: TIMET, TIMETAL 6-4 Data Sheetarchived copy.

Specific heat of Titanium Ti-6Al-4V

The specific heat capacity of Titanium Ti-6Al-4V is 580 J/kg·K (0.139 BTU/lb·°F). Basis: typical, 20 °C. Source: TIMET, TIMETAL 6-4 Data Sheetarchived copy.

Coefficient of thermal expansion of Titanium Ti-6Al-4V

Titanium Ti-6Al-4V expands 9 µm/m·K (5 µin/in·°F): a 100 mm part grows 45 µm over a 50 °C rise. Basis: typical, mean 0-100 °C. Source: TIMET, TIMETAL 6-4 Data Sheetarchived copy.

Thermal diffusivity of Titanium Ti-6Al-4V

Computed from the conductivity, density and specific heat (k / ρc): 2.57 mm²/s, how fast a temperature change spreads through it.

Melting point of Titanium Ti-6Al-4V

Titanium Ti-6Al-4V melts at 1,630–1,650 °C (2,966–3,002 °F). Basis: melting range. Source: TIMET, TIMETAL 6-4 Propertiesarchived copy.

Maximum service temperature of Titanium Ti-6Al-4V

The maximum service temperature of Titanium Ti-6Al-4V is 400 °C (752 °F). Basis: upper recommended use temperature. Source: TIMET, TIMETAL 6-4 Propertiesarchived copy.