Materials / Plastic

Plastic PEEK

Plastic PEEK (bulk) strength, stiffness, density and thermal properties, with their source.

A bracket in Plastic PEEK, smooth finish.

Mechanical
Yield strength98MPa1
Compressive strength125MPa1
Flexural strength165MPa1
Elongation at break25%1
Young's modulus (stiffness)4GPa1
Density1,300kg/m³1
Strength to weight75.4kN·m/kg
Stiffness to weight3.08MN·m/kg
Poisson's ratio0.382
Shear modulus1.45GPa
Bulk modulus5.56GPa
Speed of sound1,754m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic PEEK
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic PEEK
Strength against densityHigher and further left: stronger for its weight
Thermal
Thermal conductivity0.29W/m·K1
Thermal expansion55µm/m·K1
100 mm part over a 50 °C swing275µm growth
Specific heat2,200J/kg·K3
Heats up and cools (diffusivity)0.101mm²/s
Thermal shock resistance80.1W/m
Melting point343°C1
Glass transitiononset143°C1
Max service temperatureUL 746B RTI240°C1
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic PEEK
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Plastic PEEK
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Sources3 documents: Victrex
Values for
Bulk polymer (molded or machined). Victrex PEEK 450G (unreinforced, injection moulded), Victrex TDS rev. March 2026; Poisson from Victrex fluid-management flyer (2020-07)
  1. 1
    VICTREX PEEK 450G Technical Data SheetVictrexYield strength: typical, tensile yieldCompressive strength: typical, 23 CFlexural strength: typical, flexural stress at yield, 23 CElongation at break: typical, at breakYoung's modulus (stiffness): typical (nominal)Density: typical (crystalline)Thermal conductivity: typical, average, 23 CThermal expansion: average of flow/cross-flow, below Tg (<143 C)Melting point: typical, DSCGlass transition: onset (midpoint 150 C)Max service temperature: UL 746B RTI, mechanical strength (continuous use index)
  2. 2
    VICTREX PEEK for Use in Fluid Management (2020)VictrexPoisson's ratio: typical
  3. 3
    VICTREX PEEK 450G Technical Data Sheet (2012)Victrexarchived copySpecific heat: typical, 23 °C, DSC (Victrex PEEK 450G TDS, revision Jul 2012)

Thermal properties of Plastic PEEK

Thermal conductivity of Plastic PEEK

Plastic PEEK has a thermal conductivity of 0.29 W/m·K (0.168 BTU/hr·ft·°F). Basis: typical, average, 23 C. Source: Victrex, VICTREX PEEK 450G Technical Data Sheet.

Specific heat of Plastic PEEK

The specific heat capacity of Plastic PEEK is 2,200 J/kg·K (0.525 BTU/lb·°F). Basis: typical, 23 °C, DSC (Victrex PEEK 450G TDS, revision Jul 2012). Source: Victrex, VICTREX PEEK 450G Technical Data Sheet (2012)archived copy.

Coefficient of thermal expansion of Plastic PEEK

Plastic PEEK expands 55 µm/m·K (30.6 µin/in·°F): a 100 mm part grows 275 µm over a 50 °C rise. Basis: average of flow/cross-flow, below Tg (<143 C). Source: Victrex, VICTREX PEEK 450G Technical Data Sheet.

Thermal diffusivity of Plastic PEEK

Computed from the conductivity, density and specific heat (k / ρc): 0.101 mm²/s, how fast a temperature change spreads through it.

Melting point of Plastic PEEK

Plastic PEEK melts at 343 °C (649 °F). Basis: typical, DSC. Source: Victrex, VICTREX PEEK 450G Technical Data Sheet.

Glass transition temperature of Plastic PEEK

Plastic PEEK softens at its glass transition, 143 °C (289 °F). Basis: onset (midpoint 150 C). Source: Victrex, VICTREX PEEK 450G Technical Data Sheet.

Maximum service temperature of Plastic PEEK

The maximum service temperature of Plastic PEEK is 240 °C (464 °F). Basis: UL 746B RTI, mechanical strength (continuous use index). Source: Victrex, VICTREX PEEK 450G Technical Data Sheet.