| Mechanical | |
|---|---|
| Yield strength | 63.1MPa1 |
| Ultimate tensile strength | 63.1MPa1 |
| Flexural strength | 82.9MPa1 |
| Elongation at break | not sourced |
| Young's modulus (stiffness) | 2.33GPa1 |
| Density | 1,140kg/m³1 |
| Strength to weight | 55.4kN·m/kg |
| Stiffness to weight | 2.04MN·m/kg |
| Poisson's ratio | base material0.42 |
| Shear modulus | 0.833GPa |
| Bulk modulus | 3.89GPa |
| Speed of sound | 1,430m/s |
| Thermal | |
|---|---|
| Thermal conductivity | base material0.33W/m·K3 |
| Thermal expansion | base material98–102µm/m·K3 |
| 100 mm part over a 50 °C swing | 500µm growth |
| Specific heat | base material1,700J/kg·K3 |
| Heats up and cools (diffusivity) | 0.17mm²/s |
| Thermal shock resistance | 53.6W/m |
| Melting point | 188°C1 |
| Glass transition | 55.1°C1 |
| Max service temperature | HDT 0.455 MPa89.2°C1 |
Sources3 documents: UltiMaker, Covestro, BASF
- Values for
- 3D printed (FDM). Ultimaker Nylon, 3D-printed specimens, XY (flat), conditioned >=24 h at room temperature; Ultimaker S5 Pro, engineering intent profile, 0.15 mm layer height, AA 0.4 print core, 100% infill, Cura 4.9, printed one-at-a-time, conditioned >=24 h at room temperature. TDS v2.00, April 20, 2022.
- 1Ultimaker Nylon Technical Data Sheet, v5.00UltiMakerarchived copyYield strength: typicalUltimate tensile strength: typical, peak stress (= stress at yield)Flexural strength: typicalYoung's modulus (stiffness): typicalDensity: typicalMelting point: typicalGlass transition: typicalMax service temperature: HDT 0.455 MPa (printed specimens)
- 2Engineering Polymers Part and Mold Design: Thermoplastics, A Design GuideCovestroPoisson's ratio: base material: unfilled polyamide (PA), conditioned, maker design-guide family value (Covestro Table 3-1)
- 3Ultramid (PA) Product RangeBASFThermal conductivity: base material: unreinforced BASF Ultramid PA66 (A3K) and PA6 (B3S), 23 C (same value for both)Thermal expansion: base material: unreinforced BASF Ultramid PA66 (A3K, 98) and PA6 (B3S, 102), 23-55 CSpecific heat: base material: unreinforced BASF Ultramid PA66 (A3K) and PA6 (B3S), 23 C (same value for both)
Plastic Nylon is 3D printed: its properties depend on build direction and print settings; these are typical values.
Thermal properties of Plastic Nylon
Thermal conductivity of Plastic Nylon
Plastic Nylon has a thermal conductivity of 0.33 W/m·K (0.191 BTU/hr·ft·°F). Basis: base material: unreinforced BASF Ultramid PA66 (A3K) and PA6 (B3S), 23 C (same value for both). Source: BASF, Ultramid (PA) Product Range.
Specific heat of Plastic Nylon
The specific heat capacity of Plastic Nylon is 1,700 J/kg·K (0.406 BTU/lb·°F). Basis: base material: unreinforced BASF Ultramid PA66 (A3K) and PA6 (B3S), 23 C (same value for both). Source: BASF, Ultramid (PA) Product Range.
Coefficient of thermal expansion of Plastic Nylon
Plastic Nylon expands 98–102 µm/m·K (54.4–56.7 µin/in·°F): a 100 mm part grows 500 µm over a 50 °C rise. Basis: base material: unreinforced BASF Ultramid PA66 (A3K, 98) and PA6 (B3S, 102), 23-55 C. Source: BASF, Ultramid (PA) Product Range.
Thermal diffusivity of Plastic Nylon
Computed from the conductivity, density and specific heat (k / ρc): 0.17 mm²/s, how fast a temperature change spreads through it.
Melting point of Plastic Nylon
Plastic Nylon melts at 188 °C (371 °F). Basis: typical. Source: UltiMaker, Ultimaker Nylon Technical Data Sheet, v5.00archived copy.
Glass transition temperature of Plastic Nylon
Plastic Nylon softens at its glass transition, 55.1 °C (131 °F). Basis: typical. Source: UltiMaker, Ultimaker Nylon Technical Data Sheet, v5.00archived copy.
Maximum service temperature of Plastic Nylon
The maximum service temperature of Plastic Nylon is 89.2 °C (193 °F). Basis: HDT 0.455 MPa (printed specimens). Source: UltiMaker, Ultimaker Nylon Technical Data Sheet, v5.00archived copy.
Compare Plastic Nylon with
Other Plastic
- Plastic Nylon vs. Plastic PLA
- Plastic Nylon vs. Plastic PETG
- Plastic Nylon vs. Plastic ABS
- Plastic Nylon vs. Plastic TPU
- Plastic Nylon vs. Plastic ABS (bulk/injection)
- Plastic Nylon vs. Plastic Polycarbonate
- Plastic Nylon vs. Plastic POM/Acetal
- Plastic Nylon vs. Plastic Nylon PA6
- Plastic Nylon vs. Plastic Nylon PA66
- Plastic Nylon vs. Plastic PEEK
- Plastic Nylon vs. Plastic PTFE
- Plastic Nylon vs. Plastic UHMWPE
- Plastic Nylon vs. Plastic HDPE
- Plastic Nylon vs. Plastic Polypropylene
- Plastic Nylon vs. Plastic PMMA
- Plastic Nylon vs. Plastic PBT GF30
- Plastic Nylon vs. Plastic PPS GF40
- Plastic Nylon vs. Plastic LCP GF30