Materials / Compare

Plastic Nylon PA6 vs. Plastic PPS GF40

Compare Plastic Nylon PA6 vs. Plastic PPS GF40 strength, stiffness, weight and thermal properties.

Plastic Nylon PA6Bulk polymer (molded or machined)
Plastic PPS GF40Bulk polymer (molded or machined)
MechanicalPlastic Nylon PA6Plastic PPS GF40
Yield strength90MPa1not given (tensile used)
Ultimate tensile strengthnot stated (yield given)tensile strength195MPa2
Flexural strengthnot sourced285MPa2
Elongation at break10%15.26x more ductilestrain at break1.9%2
Young's modulus (stiffness)3.5GPa114.7GPa24.2x stiffer
Density1,130kg/m³146% lighter1,650kg/m³2
Strength to weight79.6kN·m/kg118kN·m/kg48% higher
Stiffness to weight3.1MN·m/kg8.91MN·m/kg2.88x higher
Poisson's ratiobase material0.430.354
Shear modulus1.25GPa5.44GPa4.36x stiffer in shear
Bulk modulus5.83GPa16.3GPa2.8x higher
Speed of sound1,760m/s2,985m/s1.7x faster
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic LCP GF30Plastic Nylon PA6Plastic PPS GF40
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic LCP GF30Plastic Nylon PA6Plastic PPS GF40
Strength against densityHigher and further left: stronger for its weight
ThermalPlastic Nylon PA6Plastic PPS GF40
Thermal conductivity0.33W/m·K11.65x more heat through a fin0.2W/m·K4
Thermal expansionlongitudinal102µm/m·K1parallel12µm/m·K28.5x less
100 mm part over a 50 °C swing510µm growth60µm growth8.5x less
Specific heat1,700J/kg·K1not sourced
Heats up and cools (diffusivity)0.172mm²/snot sourced
Thermal shock resistance49.9W/m144W/m2.88x more resistant
Melting pointDSC220°C1DSC280°C260 °C higher
Glass transitionnot sourcedDSC90°C2
Max service temperature87°C1HDT 1.8 MPa270°C2
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic LCP GF30Plastic Nylon PA6Plastic PPS GF40
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic LCP GF30Plastic Nylon PA6Plastic PPS GF40
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: BASF, Celanese, Covestro
Plastic Nylon PA6
BASF Ultramid B3S (PA6, unreinforced injection-moulding grade), Product Information 02/2026, dry values (ISO methods)
Plastic PPS GF40
Celanese Fortron 1140L4 (PPS, 40% glass fibre), injection moulding; FORTRON PPS Short-Term Properties Guide (PPS-012, 2016); thermal conductivity and Poisson for 40% glass-reinforced Fortron from the Fortron PPS Design Manual (PPS-050, 2013).
  1. 1
    Ultramid B3S Product InformationBASFPlastic Nylon PA6 · Yield strength: typical, dryPlastic Nylon PA6 · Elongation at break: nominal strain at break, dryPlastic Nylon PA6 · Young's modulus (stiffness): typical, dryPlastic Nylon PA6 · Density: typicalPlastic Nylon PA6 · Thermal conductivity: typicalPlastic Nylon PA6 · Thermal expansion: longitudinal, 23-55 °CPlastic Nylon PA6 · Specific heat: typicalPlastic Nylon PA6 · Melting point: DSCPlastic Nylon PA6 · Max service temperature: IEC 60216 temperature index, 20000 h
  2. 2
    Fortron PPS Short-Term Properties Guide (PPS-012)CelanesePlastic PPS GF40 · Ultimate tensile strength: tensile strength, 5 mm/minPlastic PPS GF40 · Flexural strength: flexural strength at breakPlastic PPS GF40 · Elongation at break: strain at break, 5 mm/minPlastic PPS GF40 · Young's modulus (stiffness): typical, 1 mm/minPlastic PPS GF40 · Density: typicalPlastic PPS GF40 · Thermal expansion: parallel (flow), mean -50 to 90 °CPlastic PPS GF40 · Melting point: DSC, 10 °C/minPlastic PPS GF40 · Glass transition: DSC, 10 °C/minPlastic PPS GF40 · Max service temperature: HDT 1.8 MPa
  3. 3
    Engineering Polymers Part and Mold Design: Thermoplastics, A Design GuideCovestroPlastic Nylon PA6 · Poisson's ratio: base material: unfilled polyamide (PA), conditioned, maker design-guide family value (Covestro Table 3-1)
  4. 4
    Fortron PPS Design Manual (PPS-050)CelanesePlastic PPS GF40 · Poisson's ratio: glass-reinforced Fortron PPS (class value, not grade-specific)Plastic PPS GF40 · Thermal conductivity: 40% glass-reinforced Fortron, 25 °C (not grade-specific)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Plastic Nylon PA6 stronger than Plastic PPS GF40?

Plastic PPS GF40 is stronger: its tensile strength is 195 MPa against yield strength 90 MPa for Plastic Nylon PA6 (2.17x).

Which is lighter, Plastic Nylon PA6 or Plastic PPS GF40?

Plastic Nylon PA6 is lighter: 1,130 kg/m³ against 1,650 kg/m³ for Plastic PPS GF40.

Which is stiffer, Plastic Nylon PA6 or Plastic PPS GF40?

Plastic PPS GF40 is stiffer: Young's modulus 14.7 GPa against 3.5 GPa for Plastic Nylon PA6, so the same part in Plastic PPS GF40 deflects less under the same load.

Which is lighter for the same job, Plastic Nylon PA6 or Plastic PPS GF40?

For the same stiffness or strength: Plastic PPS GF40 is lighter for a stiff rod or tie (tension), stiff beam (bending), stiff panel or plate, strong rod or tie, strong beam.

Part that must bePlastic Nylon PA6Plastic PPS GF40
Stiff rod or tie (tension)2.88x heavierlighter
Stiff beam (bending)40% heavierlighter
Stiff panel or plate10% heavierlighter
Strong rod or tie48% heavierlighter
Strong beam15% heavierlighter
Strong panel or plateabout equalabout equal

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Plastic Nylon PA6 or Plastic PPS GF40?

Plastic Nylon PA6 stretches further before it breaks: 10% elongation at break against 1.9% for Plastic PPS GF40.

Thermal

Which conducts heat better, Plastic Nylon PA6 or Plastic PPS GF40?

Plastic Nylon PA6 conducts heat better: 0.33 W/m·K against 0.2 W/m·K for Plastic PPS GF40.

Which expands less with temperature?

Plastic PPS GF40 expands less: 12 µm/m·K against 102 µm/m·K for Plastic Nylon PA6.

Related comparisons