Materials / Compare

Aluminum 6061-T6 vs. Aluminum 7075-T6

Compare Aluminum 6061-T6 vs. Aluminum 7075-T6 strength, stiffness, weight and thermal properties.

Aluminum 6061-T6Wrought
Aluminum 7075-T6Wrought
MechanicalAluminum 6061-T6Aluminum 7075-T6
Yield strength276MPa1503MPa21.82x stronger
Ultimate tensile strength310MPa1572MPa21.85x stronger
Elongation at break17%11.55x more ductile11%2
Young's modulus (stiffness)68.3GPa171GPa2
Density2,700kg/m³12,800kg/m³3
Strength to weight102kN·m/kg180kN·m/kg1.76x higher
Stiffness to weight25.3MN·m/kg25.4MN·m/kg
Poisson's ratio0.3340.334
Shear modulus25.7GPa26.7GPa4% stiffer in shear
Bulk modulus67GPa69.6GPa4% higher
Speed of sound5,030m/s5,036m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6061-T6Aluminum 7075-T6
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6061-T6Aluminum 7075-T6
Strength against densityHigher and further left: stronger for its weight
ThermalAluminum 6061-T6Aluminum 7075-T6
Thermal conductivity167W/m·K128% more heat through a fin130W/m·K3
Thermal expansion23.6µm/m·K123.4µm/m·K3
100 mm part over a 50 °C swing118µm growth117µm growth
Specific heat896J/kg·K1960J/kg·K3
Heats up and cools (diffusivity)69mm²/s43% faster48.4mm²/s
Thermal shock resistance19,159W/m26,370W/m38% more resistant
Melting pointsolidus-liquidus582–652°C1melting range532–635°C3
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6061-T6Aluminum 7075-T6
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6061-T6Aluminum 7075-T6
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Try it on a partA bracket to run stress or thermal on, free in your browserOpen in LessCADOpen in LessCAD
Sources4 documents: Kaiser Aluminum, U.S. Department of Defense
Aluminum 6061-T6
6061-T6/T651, Kaiser Aluminum typical properties; Poisson from MIL-HDBK-5J
Aluminum 7075-T6
7075-T6/T651, Kaiser Aluminum rod & bar (mechanical) and sheet/coil/plate (physical) typical datasheets; Poisson from MIL-HDBK-5J
  1. 1
    Alloy 6061 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum 6061-T6 · Yield strength: typical, 0.2% offset, .500 in dia specimenAluminum 6061-T6 · Ultimate tensile strength: typicalAluminum 6061-T6 · Elongation at break: typical, in 4D, 0.500 in dia specimenAluminum 6061-T6 · Young's modulus (stiffness): typicalAluminum 6061-T6 · Density: nominalAluminum 6061-T6 · Thermal conductivity: typical, 20 °CAluminum 6061-T6 · Thermal expansion: typical, mean 20-100 °CAluminum 6061-T6 · Specific heat: typical, at 100 °CAluminum 6061-T6 · Melting point: solidus-liquidus
  2. 2
    Alloy 7075 Rod & Bar Technical DataKaiser Aluminumarchived copyAluminum 7075-T6 · Yield strength: typical, 0.2% offset, .500 in dia specimenAluminum 7075-T6 · Ultimate tensile strength: typicalAluminum 7075-T6 · Elongation at break: typical, in 4DAluminum 7075-T6 · Young's modulus (stiffness): typical
  3. 3
    Alloy 7075 Sheet, Coil & Plate Technical DataKaiser Aluminumarchived copyAluminum 7075-T6 · Density: nominalAluminum 7075-T6 · Thermal conductivity: typical, 20 °C, T651Aluminum 7075-T6 · Thermal expansion: typical, mean 20-100 °CAluminum 7075-T6 · Specific heat: typical, at 100 °CAluminum 7075-T6 · Melting point: melting range
  4. 4
    MIL-HDBK-5J, Metallic Materials and Elements for Aerospace Vehicle Structures (2003)U.S. Department of DefenseAluminum 6061-T6 · Poisson's ratio: typical (handbook physical constant)Aluminum 7075-T6 · Poisson's ratio: typical (handbook physical constant)

Each number points to the document that states it, with the exact basis. Values without a number are computed from the sourced ones. "Not sourced" means no citable source states it (or only a specification minimum); figures computed from it are left out too.

Questions

Mechanical

Is Aluminum 6061-T6 stronger than Aluminum 7075-T6?

Aluminum 7075-T6 is stronger: its yield strength is 503 MPa against 276 MPa for Aluminum 6061-T6 (1.82x).

Which is lighter, Aluminum 6061-T6 or Aluminum 7075-T6?

Aluminum 6061-T6 is lighter: 2,700 kg/m³ against 2,800 kg/m³ for Aluminum 7075-T6.

Which is stiffer, Aluminum 6061-T6 or Aluminum 7075-T6?

Aluminum 7075-T6 is stiffer: Young's modulus 71 GPa against 68.3 GPa for Aluminum 6061-T6, so the same part in Aluminum 7075-T6 deflects less under the same load.

Which is lighter for the same job, Aluminum 6061-T6 or Aluminum 7075-T6?

For the same stiffness or strength: Aluminum 6061-T6 is lighter for a stiff beam (bending), stiff panel or plate; Aluminum 7075-T6 is lighter for a strong rod or tie, strong beam, strong panel or plate.

Part that must beAluminum 6061-T6Aluminum 7075-T6
Stiff rod or tie (tension)about equalabout equal
Stiff beam (bending)lighter2% heavier
Stiff panel or platelighter2% heavier
Strong rod or tie1.76x heavierlighter
Strong beam44% heavierlighter
Strong panel or plate30% heavierlighter

For the same stiffness or strength, mass scales with density over stiffness (or strength) raised to a power set by how the part is loaded: 1 for a rod in tension, 1/2 for a beam in bending, 1/3 for a panel (the standard material-selection indices).

Which is more ductile, Aluminum 6061-T6 or Aluminum 7075-T6?

Aluminum 6061-T6 stretches further before it breaks: 17% elongation at break against 11% for Aluminum 7075-T6.

Thermal

Which conducts heat better, Aluminum 6061-T6 or Aluminum 7075-T6?

Aluminum 6061-T6 conducts heat better: 167 W/m·K against 130 W/m·K for Aluminum 7075-T6.

Which expands less with temperature?

Aluminum 7075-T6 expands less: 23.4 µm/m·K against 23.6 µm/m·K for Aluminum 6061-T6.