Aluminum A380Aluminum A380 (die-cast) strength, stiffness, density and thermal properties, with their source.
A bracket in Aluminum A380, as-cast finish.
Mechanical Yield strength 160 MPa Ultimate tensile strength 320 MPa Elongation at break 3.5 % Young's modulus (stiffness) 71 GPa Density 2,713 kg/m³ Strength to weight 59 kN·m/kg Stiffness to weight 26.2 MN·m/kg Poisson's ratio 0.33 Shear modulus 26.7 GPa Bulk modulus 69.6 GPa Speed of sound 5,116 m/s
1k 10k 0.1 1 10 100 Density (kg/m³) Young's modulus (GPa) Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Wood Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Brass C360 Copper C110 Copper C10100 Copper C12200 Glass Steel AISI 1045 Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Magnesium AZ31B-H24 Zinc Zamak 3 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete PCB Laminate FR-4 Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Magnesium AZ91D Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Aluminum A380 Stiffness against densityHigher and further left: stiffer for its weight 1k 10k 10 100 1k Density (kg/m³) Yield strength (MPa) Plastic PLA Plastic PETG Plastic ABS Plastic TPU Plastic Nylon Rubber Wood Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Brass C360 Copper C110 Copper C10100 Copper C12200 Glass Steel AISI 1045 Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Magnesium AZ31B-H24 Zinc Zamak 3 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM PAHT-CF FDM HIPS SLA Resin Standard SLA Resin Tough 2000 SLA Resin Elastic 50A SLS PA12 Nylon DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Brick PCB Laminate FR-4 Silicon Ceramic Alumina 96% Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Magnesium AZ91D Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Aluminum A380 Strength against densityHigher and further left: stronger for its weight
Thermal Thermal conductivity 96.2 W/m·K Thermal expansion 21.8 µm/m·K 100 mm part over a 50 °C swing 109 µm growth Specific heat 963 J/kg·K Heats up and cools (diffusivity) 36.8 mm²/s Thermal shock resistance 6,669 W/m
1k 10k 0.1 1 10 100 Density (kg/m³) Thermal conductivity (W/m·K) Plastic PLA Plastic PETG Plastic ABS Plastic Nylon Rubber Wood Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Brass C360 Copper C110 Copper C10100 Copper C12200 Glass Steel AISI 1045 Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Magnesium AZ31B-H24 Zinc Zamak 3 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM HIPS SLA Resin Standard DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick PCB Laminate FR-4 Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Magnesium AZ91D Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Aluminum A380 Thermal conductivity against densityHigher and further left: spreads more heat for its weight 0.1 1 10 100 10 100 Thermal conductivity (W/m·K) Thermal expansion (µm/m·K) Plastic PETG Plastic ABS Plastic Nylon Wood Aluminum Steel Iron Titanium Steel AISI 1018 Stainless Steel 304 Stainless Steel 316 Aluminum 6061-T6 Aluminum 7075-T6 Brass C360 Copper C110 Copper C10100 Copper C12200 Glass Steel AISI 1045 Steel AISI 4340 Steel A992 Stainless Steel 303 Stainless Steel 17-4PH Aluminum 2024-T351 Aluminum 5052-H32 Aluminum 7050-T7451 Titanium Ti-6Al-4V Brass C260 Nickel Inconel 718 Magnesium AZ31B-H24 Zinc Zamak 3 Plastic ABS (bulk/injection) Plastic Polycarbonate Plastic POM/Acetal Plastic Nylon PA6 Plastic Nylon PA66 Plastic PEEK Plastic PTFE Plastic UHMWPE Plastic HDPE Plastic Polypropylene Plastic PMMA FDM ASA FDM Polycarbonate FDM HIPS SLA Resin Standard DMLS AlSi10Mg Aluminum DMLS Ti-6Al-4V ELI Titanium DMLS 316L Stainless Steel DMLS 17-4PH Stainless Steel Concrete Brick Plywood PCB Laminate FR-4 Silicon Ceramic Alumina 96% Ceramic Aluminum Nitride Aluminum 6063-T6 Aluminum 1100-O Aluminum 3003-O Aluminum ADC12 Magnesium AZ91D Solder SAC305 Plastic PBT GF30 Plastic PPS GF40 Plastic LCP GF30 Aluminum A380 Thermal expansion against thermal conductivityLower and further right: warps less when heated
Sources 2 documents: Rheocast Company, North American Die Casting Association
Values for Cast. A380 aluminium high-pressure die-casting alloy, typical properties; Rheocast Company (aluminium die caster, Germantown WI) A380 alloy data page. 1 Alloy Aluminum: A380 Rheocast Company Yield strength: typical, 25 °C Ultimate tensile strength: typical, 25 °C Elongation at break: typical Young's modulus (stiffness): typical, 25 °C Density: typical at 68 °F Thermal conductivity: typical at 68 °F Thermal expansion: typical, 68-572 °F (20-300 °C) Specific heat: typical at 68 °F
2 Product Design for Die Casting, Table 4.1: Die Casting Alloys Material Properties Comparison North American Die Casting Association archived copy Poisson's ratio: typical, as-cast, separately die cast specimens Thermal properties of Aluminum A380 Thermal conductivity of Aluminum A380 Aluminum A380 has a thermal conductivity of 96.2 W/m·K (55.6 BTU/hr·ft·°F). Basis: typical at 68 °F. Source: Rheocast Company, Alloy Aluminum: A380.
Specific heat of Aluminum A380 The specific heat capacity of Aluminum A380 is 963 J/kg·K (0.23 BTU/lb·°F). Basis: typical at 68 °F. Source: Rheocast Company, Alloy Aluminum: A380.
Coefficient of thermal expansion of Aluminum A380 Aluminum A380 expands 21.8 µm/m·K (12.1 µin/in·°F): a 100 mm part grows 109 µm over a 50 °C rise. Basis: typical, 68-572 °F (20-300 °C). Source: Rheocast Company, Alloy Aluminum: A380.
Thermal diffusivity of Aluminum A380 Computed from the conductivity, density and specific heat (k / ρc): 36.8 mm²/s, how fast a temperature change spreads through it.
Compare Aluminum A380 with