Materials / Aluminum

Aluminum 6063-T6

Aluminum 6063-T6 (extrusion) strength, stiffness, density and thermal properties, with their source.

A bracket in Aluminum 6063-T6, brushed finish.

Mechanical
Yield strength215MPa1
Ultimate tensile strength240MPa1
Elongation at break12%1
Young's modulus (stiffness)69GPa1
Density2,700kg/m³1
Strength to weight79.6kN·m/kg
Stiffness to weight25.6MN·m/kg
Poisson's rationot sourced
Shear modulusnot sourced
Bulk modulusnot sourced
Speed of sound5,055m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6063-T6
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6063-T6
Strength against densityHigher and further left: stronger for its weight
Thermal
Thermal conductivity201W/m·K1
Thermal expansion23.4µm/m·K1
100 mm part over a 50 °C swing117µm growth
Specific heat901J/kg·K2
Heats up and cools (diffusivity)82.6mm²/s
Thermal shock resistancenot sourced
Melting pointmelting range615–655°C1
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6063-T6
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 303Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Aluminum 6063-T6
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Sources2 documents: Kaiser Aluminum, Hydro
Values for
Wrought. 6063-T6 extruded tube, Kaiser Aluminum Tube & Pipe Alloy 6063 Technical Data (Rev. 05/06), typical properties; specific heat from Hydro EN AW-6063 extruded-products datasheet (Rev.4, 03/2023).
  1. 1
    Alloy 6063 Tube & Pipe Technical Data, Rev. 05/06Kaiser Aluminumarchived copyYield strength: typical, T6, 0.0625 in specimenUltimate tensile strength: typical, T6Elongation at break: typical, T6, in 4DYoung's modulus (stiffness): typicalDensity: nominal, 20 °CThermal conductivity: typical, T6, 20 °CThermal expansion: typical, mean 20-100 °CMelting point: melting range
  2. 2
    Technical Datasheet, Extruded Products: Alloy EN AW-6063 (Rev. 4, 2023)Hydroarchived copySpecific heat: typical, 20 °C (Hydro EN AW-6063)

Thermal properties of Aluminum 6063-T6

Thermal conductivity of Aluminum 6063-T6

Aluminum 6063-T6 has a thermal conductivity of 201 W/m·K (116 BTU/hr·ft·°F). Basis: typical, T6, 20 °C. Source: Kaiser Aluminum, Alloy 6063 Tube & Pipe Technical Data, Rev. 05/06archived copy.

Specific heat of Aluminum 6063-T6

The specific heat capacity of Aluminum 6063-T6 is 901 J/kg·K (0.215 BTU/lb·°F). Basis: typical, 20 °C (Hydro EN AW-6063). Source: Hydro, Technical Datasheet, Extruded Products: Alloy EN AW-6063 (Rev. 4, 2023)archived copy.

Coefficient of thermal expansion of Aluminum 6063-T6

Aluminum 6063-T6 expands 23.4 µm/m·K (13 µin/in·°F): a 100 mm part grows 117 µm over a 50 °C rise. Basis: typical, mean 20-100 °C. Source: Kaiser Aluminum, Alloy 6063 Tube & Pipe Technical Data, Rev. 05/06archived copy.

Thermal diffusivity of Aluminum 6063-T6

Computed from the conductivity, density and specific heat (k / ρc): 82.6 mm²/s, how fast a temperature change spreads through it.

Melting point of Aluminum 6063-T6

Aluminum 6063-T6 melts at 615–655 °C (1,139–1,211 °F). Basis: melting range. Source: Kaiser Aluminum, Alloy 6063 Tube & Pipe Technical Data, Rev. 05/06archived copy.

Compare Aluminum 6063-T6 with