Materials / Stainless Steel

Stainless Steel 303

Stainless Steel 303 (free-machining, annealed) strength, stiffness, density and thermal properties, with their source.

A bracket in Stainless Steel 303, brushed finish.

Mechanical
Yield strengthOutokumpu typical275MPa1
Ultimate tensile strengthOutokumpu typical585MPa1
Elongation at breakOutokumpu typical35%1
Young's modulus (stiffness)at RT200GPa1
Densityat RT7,900kg/m³1
Strength to weight34.8kN·m/kg
Stiffness to weight25.3MN·m/kg
Poisson's ratiodesign value0.32
Shear modulus76.9GPa
Bulk modulus167GPa
Speed of sound5,032m/s
1k10k0.1110100Density (kg/m³)Young's modulus (GPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcretePCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Stainless Steel 303
Stiffness against densityHigher and further left: stiffer for its weight
1k10k101001kDensity (kg/m³)Yield strength (MPa)Plastic PLAPlastic PETGPlastic ABSPlastic TPUPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM PAHT-CFFDM HIPSSLA Resin StandardSLA Resin Tough 2000SLA Resin Elastic 50ASLS PA12 NylonDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Aluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Stainless Steel 303
Strength against densityHigher and further left: stronger for its weight
Thermal
Thermal conductivityat RT15W/m·K1
Thermal expansionmean16µm/m·K1
100 mm part over a 50 °C swing80µm growth
Specific heatat RT500J/kg·K1
Heats up and cools (diffusivity)3.8mm²/s
Thermal shock resistance902W/m
Max service temperaturecontinuous871°C3
1k10k0.1110100Density (kg/m³)Thermal conductivity (W/m·K)Plastic PLAPlastic PETGPlastic ABSPlastic NylonRubberWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Stainless Steel 303
Thermal conductivity against densityHigher and further left: spreads more heat for its weight
0.111010010100Thermal conductivity (W/m·K)Thermal expansion (µm/m·K)Plastic PETGPlastic ABSPlastic NylonWoodAluminumSteelIronTitaniumSteel AISI 1018Stainless Steel 304Stainless Steel 316Aluminum 6061-T6Aluminum 7075-T6Brass C360Copper C110Copper C10100Copper C12200GlassSteel AISI 1045Steel AISI 4340Steel A992Stainless Steel 17-4PHAluminum 2024-T351Aluminum 5052-H32Aluminum 7050-T7451Titanium Ti-6Al-4VBrass C260Nickel Inconel 718Magnesium AZ31B-H24Zinc Zamak 3Plastic ABS (bulk/injection)Plastic PolycarbonatePlastic POM/AcetalPlastic Nylon PA6Plastic Nylon PA66Plastic PEEKPlastic PTFEPlastic UHMWPEPlastic HDPEPlastic PolypropylenePlastic PMMAFDM ASAFDM PolycarbonateFDM HIPSSLA Resin StandardDMLS AlSi10Mg AluminumDMLS Ti-6Al-4V ELI TitaniumDMLS 316L Stainless SteelDMLS 17-4PH Stainless SteelConcreteBrickPlywoodPCB Laminate FR-4SiliconCeramic Alumina 96%Ceramic Aluminum NitrideAluminum A380Aluminum 6063-T6Aluminum 1100-OAluminum 3003-OAluminum ADC12Magnesium AZ91DSolder SAC305Plastic PBT GF30Plastic PPS GF40Plastic LCP GF30Stainless Steel 303
Thermal expansion against thermal conductivityLower and further right: warps less when heated
Sources3 documents: Outokumpu, Steel Construction Institute, Carpenter Technology
Values for
Wrought. 1.4305 / UNS S30300, Outokumpu typical values (hot rolled, solution annealed) from 'Steel Grades, Properties and Global Standards'; max service from Carpenter CarTech 303 datasheet
  1. 1
    Steel Grades, Properties and Global StandardsOutokumpuarchived copyYield strength: Outokumpu typical (product P = hot rolled plate, transverse)Ultimate tensile strength: Outokumpu typicalElongation at break: Outokumpu typical, A5Young's modulus (stiffness): at RT (Table 12)Density: at RTThermal conductivity: at RTThermal expansion: mean, 20–100 °CSpecific heat: at RT
  2. 2
    Design Manual for Structural Stainless Steel, 4th Edition (P413)Steel Construction Institutearchived copyPoisson's ratio: design value (structural stainless steels)
  3. 3
    Carpenter Stainless Type 303 Data SheetCarpenter Technologyarchived copyMax service temperature: continuous, scaling limit

Thermal properties of Stainless Steel 303

Thermal conductivity of Stainless Steel 303

Stainless Steel 303 has a thermal conductivity of 15 W/m·K (8.67 BTU/hr·ft·°F). Basis: at RT. Source: Outokumpu, Steel Grades, Properties and Global Standardsarchived copy.

Specific heat of Stainless Steel 303

The specific heat capacity of Stainless Steel 303 is 500 J/kg·K (0.119 BTU/lb·°F). Basis: at RT. Source: Outokumpu, Steel Grades, Properties and Global Standardsarchived copy.

Coefficient of thermal expansion of Stainless Steel 303

Stainless Steel 303 expands 16 µm/m·K (8.89 µin/in·°F): a 100 mm part grows 80 µm over a 50 °C rise. Basis: mean, 20–100 °C. Source: Outokumpu, Steel Grades, Properties and Global Standardsarchived copy.

Thermal diffusivity of Stainless Steel 303

Computed from the conductivity, density and specific heat (k / ρc): 3.8 mm²/s, how fast a temperature change spreads through it.

Maximum service temperature of Stainless Steel 303

The maximum service temperature of Stainless Steel 303 is 871 °C (1,600 °F). Basis: continuous, scaling limit. Source: Carpenter Technology, Carpenter Stainless Type 303 Data Sheetarchived copy.

Compare Stainless Steel 303 with